Polycrystal films of CdS had been grown by chemical bath deposition.
The lattice constants of the grown CdS polycrystal were measured to be a_0=4.1364 A and C_0=6.7129 A.
The electron carrier concentration and hall mobility were measured by Van der ...
Polycrystal films of CdS had been grown by chemical bath deposition.
The lattice constants of the grown CdS polycrystal were measured to be a_0=4.1364 A and C_0=6.7129 A.
The electron carrier concentration and hall mobility were measured by Van der Pauw method at room temperature and their values are 4.57×10^22m^-3 and 2.14×10^-4m²/V.S respectively.
Photoluminescence spectrum produced green emission t 5140 A.